The Finishing Rolls are formed much more accurately, and revolve at a much higher speed than the roughing rolls. The latter make about 70 revolutions per minute; rolls of medium size about 140, and small rolls 230 or 240. The grooves gradually diminish in size, and the bar is passed from one to the other until the required size is attained. For small bar Iron, three rollers placed one above the other are sometimes employed. Motion being directly communicated to the centre roll, this by means of cogged wheels causes the other two to revolve in contrary directions. The heated bar is passed between the first and second rolls, and then returns from the other side between the second and third. Sheet Iron is made by passing the metal between smooth-faced rollers, which are gradually screwed nearer together as the desired thickness is being approached. Two sets are used; in the first the metal is roughed, and in the second finished off, and the surface made even and polished. The metal requires a re-heating between the processes. The sheets intended for the manufacture of tin-plate are polished by being subjected to hydraulic pressure between two smooth surfaces of cast iron. The short lengths which compose the pile, tend to produce a fibre in the bar, which in good Iron is always perceptible, however perfect the weld. In rolling fiat bars, the layers of the pile are kept horizontal, in order that the fibres may be as straight and parallel as possible. The experienced blacksmith in working up his bars always attends to the direction of the fibre, because by doing so he can make the most of his Iron and increase the strength and toughness of the articles produced. Bar Iron is known in the market by the names of Common Iron, Best Iron, Best-Best or Chain-Cable Iron. Two common defects of bar Iron are known as red-short and cold-short. Red short Iron is that which cracks when bent or punched at a red heat, although it may be sufficiently tenacious when cold. Cold-short Iron on the contrary is weak and brittle when cold, but can be worked without difficulty when hot. The quality of a bar of Iron may be tested by nicking it at one side with a chisel and then breaking it or doubling it down at the notch. If the Iron be cold-short, it will break off at once with the blow of a sledge hammer; but if the bar be of good quality, it will not break off but bend double, and those portions of it to the depth of the notch on both sides will separate a little from the body of the bar, and split up like a piece of fresh ash stick, exhibiting a clear, distinct, silky fibre. If this appearance be produced on a cold bar, and it be then raised to a cherry red heat and bent first in the direction of the pile, and then at right angles to it without cracking on the outer side of the bend, it is of excellent quality, neither red-short nor cold-short. A very small amount of phosphorus will make bar Iron brittle, so small a proportion as 0.5 per cent. having been found to make it cold-short. Sulphur has been assigned as the cause of the red-short property of wrought iron; the presence of only 0.0001 of sulphur renders the Iron very difficult to work at a welding heat.. A cold-short Iron is generally produced from a lean ore, in which case it has been found desirable to mix with it the rich red hepatic ore of Lancashire and Cumberland, which if smelted alone would produce red-short Iron. In this way two opposite defects are made to correct each other, and Iron of average strength is produced.
Boiler Plates. — In working the best boiler plates, the piling and rolling require to be carefully adjusted to each other. The length and breath of the pile should be to each other as the length is to the breath of the plate to be rolled from it. The bars composing the pile should be equally distributed, across and along its length. If care be taken in the rolling, the plate when distended to the full dimensions, will be equally strong in any direction that it may be tested. By attention to these points the manufactured plate will not possess the too common defect of being stronger in one direction than in another. Experiments have been made with a view of determining the strength of the Iron composing boiler plates; and by noting the weight necessary to pull asunder strips cut across, and comparing the results with those obtained with others cut length ways of the plate, a considerable difference is observed. The Iron has the least strength when pulled in a direction at right angles to the greatest distension by rolling. If the variation in strength is considerable, it is conclusive evidence that the plate has been improperly manufactured.
Ship-Building Plates. . — Long plates for ship-building generally possess the grain running with the length, but by an alteration in the pile they may be rolled with little fibre and of nearly uniform strength. In the long plates, however, it is not in the power of the roller to change the direction of the grain. The operation of rolling is very similar to the rolling of bars; the distension is greatest longitudinally, hence in this direction the grain lies. If piled with the major portion of the Iron across the pile, the distension of these pieces laterally neutralizes the tendency to form fibre.
Nail Rods and Hoops. — Nail rods are produced by rolling a small pile between fiat grooved roughing rolls, and, after distension laterally to a strip about six inches wide and of the thickness required for the gauge of rod produced, by rolling between plain cylindrical rolls of the hardest quality, passing through revolving cutters which shear the strip longitudinally into the required number of rods. The number of cutters on each spindle varies with the order under manufacture, from 3 to 10; the strips formerly were rolled for the production of only one length of rod, but in the more recently erected mills they are rolled of a sufficient length to cut three or four rods lengthways, producing, therefore, from each pile from 20 to 76 nail rods. The cutters are composed principally of wrought iron edged with steel, and to prevent softening by the heat communicated by the strip, are kept cool by a constant flow of water from a grated cistern fixed across the standards. — Hoops are produced by rolling a pile or billet between roughing and intermediate rolls, into a rod of the requisite sectional area, and finishing by distension laterally to the required width between plain cylindrical rolls.
Circular Saws. — The employment of saws for cutting Iron is of recent date; with the manufacture of bars in quantity, the necessity for an apparatus for cutting the ends perfectly square was very apparent, and resulted in the adoption of saws. The circular saw for cutting Iron bars measures from 3½ to 4½ feet diameter, made of either steel or wrought iron plates about 1-10th of an inch thick, mounted on an iron spindle, and stiffened, for the major part of their diameter, by stout iron face plates. A saw bench provided with friction rollers, stops, and adjusting screws, and slides for moving it backwards and forwards, is fixed in a line parallel to that of the axis of the saw; its upper surface level with the mill floor, and two inches distant from the lower edge of the saw plate. The saws are driven at a high velocity by means of belts and spur
Please Note: These web pages retain the original pagination from the publication