The plate of the Fine Metal thus formed is about ten feet long, 2½ feet broad, and 2 inches thick. A thin crust of slag forms upon its surface; but the greater portion is collected in a small pit at the lower end of the mould. As soon as one charge of metal is run out, the hearth is prepared for another. The workmen first detaches, by means of a long rod, any portions of metal that may be adhering to the sides of the furnace; he then presses down the fuel, throws in a fresh supply of coke, and levels it to the proper height; upon this he arranges six Iron pigs four parallel to the long sides of the furnace, and two across. The weight, which may vary from 20 to 30 cwt., takes about two hours in refining, and the loss is from 13 to 17 per cent. In about a quarter of an hour the Iron melts down, and falls in drops through the blast to the bottom of the furnace. When the decarbonisation is thought to be sufficiently advanced, the hole is opened, and the metal allowed to flow into the mould. A considerable quantity of cold water is thrown upon it, whereby it becomes extremely brittle and sonorous. The slags are then broken in pieces for the puddling furnace. About 10 tons of cast Iron may be passed through the refinery in the course of 24 hours, with the consumption of from 4 to 5 cwt. of coke for each ton of metal refined. For the better kinds of Iron, such as that used for the manufacture of tin plates and iron wire, where the tenacity of the pure metal is required, coke is too impure a fuel; charcoal is therefore used; but as with this fuel the metal collects into clots or lumps, they are formed into a bloom which is conveyed in the helve and flattened into thin plates, preparatory to being finished in another furnace.
The Puddling Furnace has a hearth about 6 feet long and 4 feet wide at the widest part, and tapers to about 20 inches towards the chimney; it is made of fire-brick set on edge, or a plate of cast Iron, covered with a layer of slag, and is made to incline to allow the escape of the slags formed during the process of puddling. It is heated by a fire from which it is separated by a bridge 10 inches high. The fire bars are made moveable for the purpose of removing the clinkers; and the draught is determined, through the furnace, by a chimney from 30 to 50 feet high, furnished at the top with a damper, which can be raised or lowered by means of a chain and lever. Openings communicate with the grate and hearth; the latter is chiefly used for working the metal with an Iron bar during the process of puddling; another opening near the chimney is used for charging and cleaning out the furnace. The whole is strongly built, encased with cast Iron. The charge of fine metal is piled up on the sides of the hearth, until it nearly touches the dome, the centre of the sole being left clear for working the charge, and allowing the hot air to circulate about it. A portion of rich slag and iron scales is added; the doors and the damper at the top are closed, and fresh fuel is added to the fire. In about half an hour the metal begins to melt and flow on the bottom of the hearth. The man removes a small iron plate from a hole in the working door, passes in an iron rod, and stirs up the molten metal so as to expose fresh surfaces to the oxidizing influence of the draft, and moves it further from the bridge, to prevent the whole of the charge from running together. When the charge is brought into a uniform pasty mass, the fire is lowered by gradually closing the damper, and, if necessary, throwing a little water into the furnace. The metal now, from the escape of carbonic oxide gas, assumes the appearance of boiling, and the gas burns at the surface with its characteristic blue flame. The metal is kept constantly stirred with an iron paddle, so as to expose fresh surfaces to the action of the gases; the direct action of the atmosphere is avoided as much as possible by keeping the working door closed, otherwise the metal would be too much oxidized. By continuing to work the metal it loses its consistency, and becomes sandy, or, as the workman calls it dry; the evolution of carbonic oxide ceases, but the puddler continues to work the metal until it appears uniformly granular. The fire is then gradually urged, and the increased temperature causes the sandy particles to agglutinate; the Iron is then said to work heavily. A portion of the slag is run off through the flosshole, and the man then proceeds to ball up, or to form the Iron into balls. For this purpose he attaches a small portion to the end of his paddle, and, rolling it round, other fragments weld on to it. When a ball of 60 or 70 lbs. weight has been formed, it is detached from the paddle, and another is formed in a similar manner. When the whole of the charge has been balled, it is moved into the hottest part of the furnace, by means of a kind of rake called a dolly, and the fire is urged so as to weld the metallic particles. Each ball is then lifted out of the furnace by means of heavy tongs, and conveyed to the shingling hammer, or to the squeezer, where an iron rod is welded to it by way of a handle; the slag is pressed out, and the metal consolidated. The whole operation of Puddling occupies about two hours and a half. At the end of the first 20 or 25 minutes, the metal begins to fuse, and in another hour is completely reduced to a sandy state, in which it is kept for another half hour, when the balling is commenced and occupies about the same time. From 10 to 11 charges, of 3½ to 5 cwt. each are passed through the furnace in the course of 24 hours. The fine metal loses about 9 per cent in the puddling, and occasions the consumption of about its own weight of Coals.
In referring to the process of puddling, Mr. Corbet, of Clayton, Manchester, an acknowledged authority, says — "That nearly all pig Iron is covered with sand more or less; that sand melts and combines with the tap cinder, at the same time a portion of fire-brick melts down into the heat and combines with the cinder, the latter being calcined and brought back receives another portion of sand, so that the silex begins to predominate, and every pound of it will waste 4 lbs. of Iron to neutralise itself and form a silicate, so that it is the silex that is the cause of such a waste in yield. Now, if an Ironmaster will put 2 or 3 lbs. of common salt into every puddled heat, the chlorine, being an oxidizing agent, is in its legitimate place in the puddling furnace, and the soda from the salt being such a strong alkali will combine with the silex, and form a neutral compound, and by following it up a few weeks, instead of the silex predominating and wasting the Iron, the alkali will predominate, and feed the Iron; and any Ironmaster who has worked the last six months without salt, if he will work the next six months with salt, he will find such a difference in the yields in his books that he will hardly believe his own eyes when he sees it."
Please Note: These web pages retain the original pagination from the publication