which the slag flows. The fauld is stopped up with sand, and the furnace bottom covered with powdered lime or charcoal dust. Ignited coke is then allowed to fall down, and is brought forward with iron bars nearly to a level with the dam. The tuyere holes are opened, and lined with a soft mixture of fine clay and loam. The blast is first introduced through a small discharge pipe, and afterwards a larger one is used. In about two hours after blowing, a considerable quantity of lava will be accumulated; this is admitted to all parts of the hearth, and glazes the surfaces of the fire stone. It then rises to a level with the notch in the dam plate, and flows over. When the metal has risen nearly to a level with the dam, it is let out by cutting away the hardened loam of the fauld, and conveyed by a channel made in the sand in front of the furnace, to the place where it is cast into pigs. In six days from the commencement of blowing, the furnace will have wrought itself clear, at which time the charge will be in the following proportions — 400 lbs. of coke, 336 lbs. of clay ironstone, and 100 lbs. of limestone. This charge is thrown into the furnace every hour; and having been thrown in at the top of the furnace, gradually descends until it reaches the upper part of the boshes. In the cone the heat is not very great; near the boshes it is considerable, and in the hearth it is at its maximum, for here the oxygen of the blast meets the fuel, and produces the most vivid combustion. The chemical changes which go on in different parts of the furnace, have been tested by collecting the gases at various distances below the throat or tunnel-hole, by passing a wrought iron pipe to the depth at which it was required to examine the products of combustion. The Iron, deprived of its oxygen, reaches the upper part of the hearth; and the intense heat, caused by the action of the blast upon what remains of the fuel, completely fuses both the iron and the silicates, and they pour down into the crucible beneath.
But in the numerous analysis of blast furnace gases, the absence of all information respecting the gases in the region of the boshes is very remarkable. The difficulty of piercing the greater thickness of work in this locality has probably deterred the experimenters from collecting the gases from within the boshes, hence the gap in the analysis; and to this circumstance may be ascribed many of the inconsistencies observed in the analysis, and for which no explanation is given, though they vitiate the conclusions drawn by the experimenters of the chemical action of the blast furnace. The construction of the hearth allows the melted products to fall rapidly through the blast; but on reaching the crucible, the fused products arrange them selves in the order of their density. The Iron occupying the lowest part, and being covered by the silicates, is completely protected from all oxidizing influence. The silicates or slag occupy a volume five or six times greater than that of the Iron, so that as it rises to the level of the dam-plate, it flows over, and passes down the inclined plane to the ground, and when cold is removed by means of pointed iron levers. The Iron slowly accumulates in the crucible, and in the course of about twelve hours the furnace is tapped; the liquid metal is then drawn off, and allowed to run into sand moulds arranged on the floor of the workshop, forming large ingots, called pigs. When the crucible is emptied, the clay plug forming the tap is restored, the blast is put on, and the operations of the furnace proceed as before, day and night, week-day, Sunday, and holiday, for years together, until requiring repair. The quantity of pig Iron produced in an ordinary blast furnace from clay ironstone, and coke as the fuel, is subject to considerable irregularity, whilst that produced by the employment of charcoal is generally of uniform quality; but the experience of years in the use of coke as a fuel, has enabled the skilful Iron-master to classify the pig Iron thus produced into about six different varieties. The first three, termed No. 1, No. 2, and No. 3, are considered as Foundry Metal; they contain carbon in different degrees, but all of them in a higher degree than those selected for making bar or malleable Iron. No. 1 is saturated with carbon, the effect of which is to produce a soft Iron, very fluid when melted, so that it will adapt itself perfectly to the shape of the mould, and is hence used for small and ornamental castings. It is also so soft as to yield readily to the chisel. No. 2 contains less carbon than No. 1 it is not so soft when cold, nor so fluid when melted; but being harder and stronger, is preferred for those parts of machinery which require strength and durability. The quantity of carbon contained in these two sorts renders them unfit for being manufactured into bars; but No. 3, or Dark- Grey Iron, containing less carbon than No. 1 or No. 2, can be used either for the forge or for the foundry. It is employed in heavy castings, such as tram-plates, heavy shafts, wheels, cylinders of steam engines, &c. The next quality is called Bright Iron, from its being of a lighter colour and of a brighter lustre than the foregoing varieties. It is used for large castings, but is not sufficiently fluid for fine work. A fifth variety is Mottled Iron, the fracture of which is mottled with grey and white. It is too thick and brittle for the foundry, and its use is confined to the forge. The last variety is called White Iron, from its silvery white colour. It is quite unfit for casting on account of its thickness and extreme brittleness. It contains a smaller proportion of carbon than any other sort of pig Iron; indeed, its production often depends upon a deficiency of fuel in the charge. The quality of the metal can be judged of before it is run from the furnace, by the colour and form of the scoriae, the colour of the crust upon the working bars, and the quantity of carburet attached to it. The different kinds of Iron present also different phenomena in flowing out of the furnace.
The quantity of coke required to produce a given weight of cast Iron depends upon the nature of the ores, the combustible employed, the form and dimensions of the furnace, &c. When charcoal is the fuel used, every part of metal produced requires, on an average, 1½ parts of fuel for its preparation. In Staffordshire, from 3½ to 4 tons of Coals, including that employed for roasting the ore, are required for the production of one ton of cast Iron. In Wales the Coal produces a larger percentage of coke than that which is obtained in the above locality, and each ton of cast Iron is there calculated to require for its manufacture 3 tons of Coal, equal to about 2.1 tons of coke, in which form it is supplied to the furnace.
Hot Blast.
The important discovery of the employment of hot air instead of the ordinary cold air of the atmosphere, in supplying the blast of furnaces for smelting and founding Iron, is due to Mr. Neilson, of Glasgow. The enormous quantity of air injected into a blast furnace to promote the combustion of the fuel, must have its own temperature raised before its oxygen can combine with the carbon of the fuel in the way of combustion. In fact one portion of the heat of the furnace is expended in raising the air to the temperature necessary for the combustion of the remaining fuel; a second portion of the heat is
Please Note: These web pages retain the original pagination from the publication