Potash This valuable plant food, occurs as Sylvine KCl, sp. gr. 1.98, Carnallite KCl MgCl2. 6 H2O sp. gr. 1.60, Langbeinite, 2MgSO2 K2SO4 Polyhalite K2SO4 MgSO4 2CaSO4 2H2O sp. gr. 2.78, and Kainite, MgSO4 KCl 3H2O sp. gr. 2.1. As all these salts, with the exception of Polyhalite, are readily soluble, it is difficult to effect any concentration in water unless a saturated solution is employed. Apart from solution and recrystallisation, together with fractional crystallisation for the separation of sodium and potash salts, flotation is now employed to make the bulk of the preliminary separation of Halite from Sylvine. The operation is carried out in a brine saturated with both salts and either Sylvine or Halite can be removed, using froth flotation for minus 35 mesh material and table agglomeration for coarser salts. Halite is floated from Sylvine using fatty acids, their soaps, or naphthenic and tar acids as collectors, lead or bismuth salts as activators, and higher alcohol sulphates as collector assisting reagents. Sylvine, on the other hand, can be floated from Halite and clay using anionic type wetting agents, such as the sulphates of aliphatic alcohols containing eight to twelve carbon atoms with small quantities of cresylic acid as a frother. Amine salts with eight to twelve carbon atoms are also reported as satisfactory collectors and protective colloids, such as glue and starch may be desirable to assist in selectivity when this type of collector is employed. The use of sodium hexametaphosphate has also been recommended for the depression of Halite when Sylvine is to be floated. At the Potash Company of America plant, situated at Carlsbad, New Mexico, the Halite is floated from the Halite-Sylvine brine, using 0.5 lb. per ton of Coco oil or other brine soluble soap, gas oil amounting to 0.2 to 0.5 lb., 0.2 lb. Cresol, 0.25 to 0.5 lb. Caustic starch, and 0.25 lb. lead chloride per ton. The cresol is reported to be non-frothing in brine, but tends to decrease the volume of froth and make it more brittle, thereby increasing the selectivity. The flowsheet is shown in Fig. 10. At the Union Potash Co., also at Carlsbad, the Sylvine is floated from Halite, using froth flotation for minus 35 mesh material, and table flotation for 8 mesh down to 35 mesh. The reagents used are said to be 0.3 to 0.5 lb. of an amine with 16 to 18 carbon atoms, and 0.25 lb. of pine oil in froth flotation. Crude Langbeinite is also treated in the plant, but this is simply washed to remove Halite in solution and Sylvine added so that base exchange takes place, forming magnesium chloride and potassium sulphate crystals. Recently experimental work has been carried out on the use of sink and float in a brine medium, and it is reported that the cyclone type of heavy media washer has been successful. Talc Pure Talc has an approximate composition of H2Mg3(SiO3)4, but commercial Talc is often a mixture with other minerals, for instance, fibrous Talc owes its structure to Tremolite, whilst impurities such as Dolomite render it gritty, and Serpentine or Chlorite darken the colour. It is used chiefly in the paint industry, but, ceramics, paper, rubber, roofing felts, safety fuse and foundry facings also consume a certain amount. Concentration is not extensively practiced, most Talcs being hand picked and ground either wet or dry, but flotation is now being employed increasingly for the preparation of high grade material and is being successfully carried out in this country, as well as in the United States, Canada, Africa and the U.S.S.R. In general, talc flotation is preceded by a dry mill recovery which scalps off the high grade. A neutral circuit is usual with a short chain amine, reagent 801, Emulsol X-1, fuel oil or kerosene and an alcohol or pine oil as a frother. At the Eastern Magnesia Talc Co., some 1 lb. per ton of Ultrawet, a sulphonated petroleum fraction is the sole reagent, whilst pine oil alone often floats foliated talc, but for fibrous varieties amines are better. Vermiculite This name is given to a group of minerals which evolve water and expand tremendously, up to 16 times in one direction, when heated. They usually have the appearance of bronze mica, but the plates are soft and inelastic. Their chief use is as heat insulators, paint extenders, lubricants, decorative finishes and acoustic plasters, and are chiefly produced in the States, but deposits are also worked in South Africa and the U.S.S.R. Treatment usually consists of crushing, hand picking, screening and drying. Any fine material produced may be floated in the same way as mica is treated, whilst somewhat coarser material can be treated by table-flotation. The reagents used consist of sulphuric acid, long chain amines, fuel oil as a collector-assisting reagent and pine oil or cresylic acid as a frother. As in mica flotation, aluminium sulphate assists in making a high grade concentrate, as it depresses granular silicates. It is reported that Vermiculite can also be floated with the new Cyanamid "800" reagents. Dry concentration involving winnowing and screen ing has also been employed satisfactorily, and electrostatic separation is used at the plant of The Universal Zonolite Insulating Co., situated at Libby, Montana. Here the gangue constituents are Kyanite and Pyroxenite, and the ore carries 32 per cent. Vermiculite. Concentration brings the grade up to 96 per cent., with only 2.5 per cent. in the tailing, recovery being about 96 per cent. The feed is screened 2 to 6 and 26 mesh, each fraction going to separate units capable of treating 12 tons per hour. SELECTED REFERENCES:
Drawings and Photographs accompanying the article
Article reproduced from a copy of the magazine held at National Mining Museum Scotland, Newtongrange, Midlothian.
|
![]() |
||||||||
|
Mail: Webmaster |
Back |
Home |
Copyright © 1999-2024 by The Durham Mining Museum and its contributors Registered Charity No: 1110608 Page last updated: 17 Jan 2023
|
Search |
|
|||