Museum Entrance Museum
Museum
Friends of Durham Mining Museum
Events Calendar
e-Books and Books for sale
Photograph Gallery
Document Archive
Main Document Archive
Newspaper Articles
Local Record Extracts
D.M.A. Document Archive
Transactions of I.M.E.
Miners' Welfare
N.C.B. Archive
The Colliery Engineer
The Colliery Guardian
Mine & Quarry Engineering
Mine & Quarry Engineering - Main Index
Mine & Quarry Engineering - Subject Index
Mining Journal
The Science and Art of Mining
Coal Magazine
Coal News
Coke and Gas
Master Name Index
What's new in the site
Mining
Mining History
Colliery Index
Colliery Maps
Company Overviews
Who's Who
Mineral Information
Managers Certificates
Educational Material
Bibliography
Statistics
Workers/Employee Lists
Notes for Family Historians
War Service information
Disasters
Disaster Reports
Names of those killed
Disasters in the 1700s
Disasters in the 1800s
Disasters in the 1900s
Memorials
Awards for Gallantry
On this day ...

Links to other sites of interest
Industrial Heritage Days Out
Former www.pitwork.net web site

Index to site

Contact and address details

Share Page with Social Media

Share on Facebook

Share with Reddit

Share on Delicious

Title Prev Page Return to Index Next Page Title
 
 Mine & Quarry Engineering May, 1948 

Phosphates

The chief source is phosphate rock, known sometimes as Phosphorite and consists essentially of tricalcium phosphate with varying amounts of water and small quantities of other impurities such as calcium carbonate, organic matter, fluorides, iron oxide and alumina. It has a specific gravity of from 2 to 3. Another source is Apatite, which occurs as Chlor-apatite, 3Ca3 P2O8. CaCl2, containing 89.35 per cent. tricalcium phosphate, and Fluor-apatite, 3Ca3 P2O8. CaF2, containing 92.96 per cent. tricalcium phosphate, but the commercial product is usually a mixture of both these minerals.

It is usual to state the phosphorus content, as tricalcium phosphate, called bone phosphate of lime or B.P.L. in the United States, and grades of dressed rock vary from 60 to 80 per cent. B.P.L. For comparison it is useful to remember that one pound of P2O5 is equivalent to 2.185 lb. B.P.L. and to 0.44 lb. of elemental phosphorus.

Treatment generally consists of washing in log washers to break up clay balls, followed by screening and classification for the separation of fines which usually contain the bulk of the waste material. A certain amount of picking is possible on lump ore but, in other cases, grizzley oversize may contain clay balls which can be rejected or slightly crushed and rewashed. Hard rock ore on the other hand, requires a certain degree of crushing and in this case treatment consists of successive rejection of a tailing at progressively smaller sizes with the employment of stage reduction.

All material finer than 14 to 20 mesh is deslimed and treated by frother flotation or table agglomeration which recovers about 80 per cent, of the phosphate in the fines. The addition of flotation has increased the overall recovery from about 50 per cent. to 90 per cent. but attempts to float the finest material, say minus 200-mesh have failed and indeed the presence of appreciable slime has a detrimental effect on the flotation of the more sandy material, so that desliming is an important step in present day treatment. Electro-static separation is also employed for cleaning concentrate and a higher recovery than is possible by flotation alone is claimed. In the case of Apatite, however, flotation in the presence of slime is possible and no desliming is practised in the Khibingorsk plant.

Owing to the slightly higher specific gravity of Apatite, about 3.2, it is also possible to attain a degree of concentration on tables as in the Piney River plant. The principle has also been used to a very limited extent on phosphate rock when the density differential is sufficient to make a separation.

Although much of the rock in the United States is obtained by washing, the remainder, much of which was previously rejected, is now recovered by froth flotation and table agglomeration.

Fatty acids are employed almost exclusively as collectors and, as the froth breaks down rapidly, filtering is unnecessary.

In general the pH of the pulp is maintained between 9 and 10 using lye or sodium hydroxide amounting to 0.3 to 0.6 lb. per ton with 0.3 to 1.5 lb. per ton of oleic acid and 3 to 5 lb. of light fuel oil, whilst in some cases a supplementary frother, generally pine tar oil amounting to 0.1 lb. per ton may be used.

Although oleic acid is probably the collector generally employed, other fatty acids, such as fish oil acid, seal oil and tall oil have been found to be quite suitable. Mixed carboxyhic acids, formed by the oxidation of petroleum jelly and naphthalenic acid, has also been suggested as substitutes.

The slime separation is carried out at about 200 mesh, the slime free sand being conditioned at 70 to 75 per cent, solids for a period of 4 or 5 minutes with the reagents. Two types of conditioners are commonly used, a horizontal drum type and a special modification of the usual vertical agitator type, designed to handle coarse material at a high pulp density. After conditioning, the pulp is diluted to about 30 per cent, solids before flotation. Separation is rapid and one-stage cleaning is sufficient to produce a 72 to 78 per cent, concentrate from a feed carrying 20 to 40 per cent. tricalcium phosphate. Apatite may be floated with similar reagents and is frequently more easily concentrated. In some cases, desliming is necessary, although the practice is not universal.

In the past when flotation was used, the general practice has been to float the phosphate as outlined above, but with the development of cationic reagents, two alternatives to straight phosphate flotation have become available, namely, the froth flotation of phosphate to make a rougher concentrate, followed by the flotation of residual silica with a cationic reagent, and direct froth flotation of the whole of the silica in the rock.

Although it is too early to determine the advisability of converting entire plants to straight silica flotation, there are many favourable points in this system provided thorough desliming of the flotation feed is possible in order to remove clay which impedes the flotation of quartz and other granular silicates. It is claimed that the cationic reagent will float 20,000 lb. of quartz per lb. of reagent consumed. Such treatment is best suited to the under 35 mesh material, the usual table agglomeration process being reserved for material from 14 to 35 mesh.

In the hard-rock phosphate district of Florida, the nodules range in size from 100 mesh to boulders as large as 26 ft. in diameter, in a matrix of sand, clay, finer phosphate rock and occasionally flint and calcareous rocks.

The ore usually requires some crushing and the plant of section 12 mine, flowsheet No. 4 is typical of a straightforward washing layout.

At this mine no flotation is employed, but at others the log washer overflow is deslimed and treated by table agglomeration, any material coarser than 14 mesh being ground in a rod mill operating in closed circuit with a 14 mesh screen. It will be noticed from the flowsheet that hand selection is employed at two points in order to eliminate clay balls, flint and lime rock.

At the Southern Phosphate Company's washer situated at Pauway, Florida, in the soft rock district, the phosphatic debris contains 30 per cent. B.P.L., most of which is under ½ in. and over 20 mesh so that all plus ½ in. is scalped out and discarded. Coarse nodules from ½ in. to ¼ in. are screened out without further treatment but the undersize is washed, classified making a concentrate from the first spigot, whilst the material from the remaining spigots is conditioned with fatty acid and fuel oil, and treated by table agglomeration. A recovery of 90 per cent, is reported with a concentrate containing 76 per cent. B.P.L. The flowsheet is given in Fig. 5. At the San Gully plant of the Southern Phosphate Corp., the raw pebble rock from hydraulic mining is disintegrated in log washers as well as by tumbling in a Hardinge mill with no ball load, screened and classified to reject slime and make a concentrate coarser than 16 mesh. All minus 16 mesh material is concentrated by table agglomeration. Here a finished product, a tailing and a middling are made. The middling is re-conditioned and passed over three further tables. The flowsheet is shown in Fig. 6.

At the American Agricultural Chemical Co., Carmichael, Florida, froth flotation alone is employed. Here the ore is washed, scrubbed, screened and classified, making a concentrate from the first and second spigot of a five pocket Fahrewald classifier, whilst the material from the third to fifth spigots as well as certain of the washer overflow, is deslimed in a bowl classifier and floated with soap and fuel oil in the usual manner. The rougher concentrate is a finished product whilst the scavenger froth is cleaned once and the cleaner tailing returned to the classifier.

As an example of both froth flotation and table agglomeration, combined with the removal of silica using cationic collectors, the plant of the International Minerals and Chemical Corporation, at Peace Valley, Florida, has been selected. Here some 350 to 450 cu. yd. of matrix consisting of virgin pebble phosphate is treated per hour.

The rock is mined by dragline, hydrauliced and pumped to the plant where it is screened, the oversize crushed in rolls in order to tear up clay balls, resized on screens, washed and disintegrated in log washers so that some coarse pebble phosphate can be separated by simple screening.

The minus 14 plus 35 mesh material is carefully deslimed, conditioned in a thick pulp and treated by table agglomeration, whilst all minus 35 mesh material is deslimed and treated by froth flotation to yield a rougher concentrate using a fatty acid collector. This is then thickened, agitated in a fourcell mixer with sulphuric acid to remove oleic acid coating, treated in a bowl classifier where the fatty acid overflows and finally refloated to remove residual silica using a cationic collector. The flowsheet of this plant is shown in Fig. 7.

At another plant, operated by Swift & Company, at Agricola, Florida, the matrix is sized, washed and screened to make a coarse concentrate, whilst all undersize from a 1-mm. screen is deslimed and classified in a five-spigot Fahrenwald classifier. Material from the first two spigots passes direct to concentrate bins, from the third and fourth spigots to agglomeration and that from the last spigot, together with the deslimed overflows, go to flotation.

The agglomeration plant is rather unusual in that a screen is employed instead of tables for the separation of agglomerated phosphate rock, the agglomerated material standing on an underwater screen sloping at 55 deg. with a 16 mesh opening. The undersize from this screen, however, passes to flotation for retreatment. Reagents reported comprise tall oil (a by-product in paper manufacture), sodium hydroxide and fuel oil. (See flowsheet, Fig. 8.)

Conveyor belt separators have also been employed where the agglomerated phosphate is washed off the surface of a thick layer of pulp by sprays of water. At the same time ploughs turn the load on the belt so bringing agglomerated material into contact with air before subjecting it to the action of the water sprays.

Electrostatic separation is being used at the Pierce plant of the American Agricultural Chemical Co., where two double 9-electrode Johnson separators are used to up-grade flotation concentrate. The first six electrodes act as roughers and are positively charged with 15,000 volts, whilst the last three act as cleaners and are charged with 17,000 volts. Each duplex separator has a capacity of 16.8 tons per hour and the feed is under 35 mesh being dried at 165 deg. F. From a feed assaying 71.74 per cent. B.P.L., the final concentrate carries 76.89 per cent, with a tailing of 14.86 per cent. The percentage of insolubles in the feed amounts to 11.97 per cent., but only to 5.44 per cent. in the separator concentrate.

It is claimed that by using this double treatment, it is possible to recover 90 per cent., instead of about 80 per cent., as is the case with straight flotation, whilst it has been suggested that the reagent film on the phosphate is utilised to make a cleaner separation than is possible with either electrostatic separation alone or flotation.

Very few Apatite concentration plants exist and probably the largest is at Khibinogorsk, in the U.S.S.R., where a very large body of nepheline syenite containing Apatite is being treated by flotation. Local reagents made from peat tar and seal oil are used, as they are cheap in spite of their tendency to produce excessive froth in sub-aeration cells. For this reason oleic acid is often employed in its stead, and the peat tar product reserved for the pneumatic cells. A recovery of 95 per cent, is made in a concentrate assaying 39.5 per cent. P2O5 from a feed containing a maximum of 28 per cent. P2O5 (or 65 to 70 per cent, of Apatite). The flowsheet of the flotation section is shown in Fig. 9.

In Sweden, Apatite occurs as an impurity in iron ore and a semi-commercial plant is in operation, making a 74 to 85 per cent, recovery of the phosphate as a product containing 30 to 40 per cent. P2O5. A middling carrying 42 per cent. iron and 1 per cent. phosphoric acid is made, but as the latter occurs very largely in the fines, it is removed by screening.

A purely gravity plant is in operation for the recovery of Apatite at Piney River, Va., U.S.A., which handles 100 tons per day. The ore carries Ilmenite and Apatite and both are recovered by treatment on tables. The Ilmenite concentrate assays about 42 per cent. TiO2 and the Apatite product 40 per cent. P2O5, but the recovery of this mineral is low, being only 55 per cent.

Briefly, the flowsheet consists of grinding to 35 mesh in a rod mill in closed circuit with a screen, desliming in a cone classifier, and classifying. The first spigot is drawn as an Ilmenite concentrate and remaining spigots treated on tables. The table concentrates are finally passed through two magnetic separators in series to remove residual Ilmenite and table middling is returned to the rod mill circuit.

Drawings and Photographs accompanying the article

 

Prev Page Return to Top of Page Next Page

Article reproduced from a copy of the magazine held at National Mining Museum Scotland, Newtongrange, Midlothian.

 

mail
Mail:
Webmaster
Back
Back
Home
Home
Open Government Licence   Contains public sector information licensed under the Open Government Licence v3.0.

Copyright © 1999-2024 by The Durham Mining Museum and its contributors
Registered Charity No: 1110608
Page last updated: 17 Jan 2023

Privacy Policy
 
Terms & Conditions
 
Search
Search
Print
Print