CHAPTER VI.
MANUFACTURE OF STEEL — THE ORDINARY PROCESS; PROCESSES ON THE CONTINENT; DIFFERENT KINDS OF STEEL. TILTING. CAST STEEL — PROCESS OF CASTING. DAMASK STEEL. BESSEMER'S PROCESS OF "MANUFACTURING STEEL WITHOUT FUEL;" ITS SUCCESS; BESSEMER'S PROCESS ADOPTED BY MANUFACTURERS AT SHEFFIELD, DURHAM, ETC.; CAST STEEL BRIDGE; BESSEMER STEEL THE CHEAPEST OF ALL THE MALLEABLE METALS.
Manufacture Of Steel.
When a pig of Iron is rolled into bars, or rods, or sheets, it is ready to be applied to purposes which may indeed be said to be innumerable. For the manufacture of Steel, charcoal Iron of the best quality only is employed. The Iron most approved for this purpose is obtained from Sweden, and marked with the letter L in a circle, hence called Hoop L. Inferior Swedish Iron is known by the marks C and a crown, D and a crown; the Steinbuck,/I>, and the W and crowns. Excellent Iron of this quality is also manufactured in Russia and Madras, and in our own country at Ulverstone.
Iron in its manufactured state is never entirely free from carbon and other substances. The carbon appears to be only mechanically mixed with the metal, a peculiar process being required to effect a chemical union between the two, the result being a carburet of Iron or Steel. Less than ½ percent. of carbon chemically combined with Iron develops those remarkable properties which distinguish Steel from Iron, and adopt it to purposes for which Iron is inadequate. Thus Steel is so much harder than Iron that it will cut and file it; Steel will scratch the hardest glass; strike sparks with siliceous stones; it is denser than Iron, has a finer grain, assumes a brighter and whiter lustre when polished, acquires greater elasticity, retains magnetism more permanently, and does not rust so easily. When heated it assumes various beautiful tints of colour, and if suddenly cooled it becomes harder, more brittle, and less pliable than Iron. Indeed, the chief value of Steel depends upon the ease with which it can be hardened and tempered to any degree between extreme hardness and softness. The quantity of carbon required to render Iron steely, depends greatly on the purity of the metal; shear steel after tilting contains from 1 to 1.5 per cent, of carbon ; with more than 1.75 per cent. the steel cannot be welded. Iron with 2 per cent. of carbon cannot be forged; but with 1.9 per cent. of carbon, Iron may with care be worked under the hammer; and this appears to be the extreme point of carbonisation, beyond which Steel is converted into cast Iron.
In this country Steel is manufactured by the addition of carbon to pure malleable Iron by what is called the process of cementation. In Germany, Styria, and Silesia, Steel is made by depriving some of the better kinds of cast Iron of the excess of carbon contained in them, one portion being got rid of by oxidation, while another portion is made to combine chemically with the fused mass, the process being thus directly the reverse of that followed in England. The Cementing Furnace in which Iron is converted into Steel in this country, resembles, externally, an ordinary glass-house, and consists of a cone or hood 30 or 40 feet high, serving to shelter the furnace within and also to carry off the smoke of the fuel. Within the furnace are two chests or troughs, in which the bars of Iron to be converted are buried in pounded charcoal. These troughs are made of fire-tiles, or fire-stone grit, and are capable of holding from 8 to 12 tons of bar Iron. They are from 8 to 15 feet long, and from 26 to 36 inches in width and depth ; but those of small capacity are said to produce the most uniform quality of Steel. Below and between the troughs, and extending their whole length, is a grate open at each end, where it is supplied with fuel, and the fire is kept up as equally as possible during the process, the flame being directed equally round the troughs by a number of air holes and flues leading to the chimneys. The draught is further aided by an opening in the middle of the arch of the furnace. The troughs are, of course, filled before the fire is lighted, and the preparation of hard charcoal dust, called cement, varies with different Steel converters; charcoal made from hardwood is preferred, but soot is sometimes used, as also a proportion of ashes, say about 1-10th, and a little common salt. The workman sifts this mixture to the depth of two inches over the bottom of the troughs; puts in the bars upon their narrow edges, with a space between every two bars of from &189; to ¾ of an inch ; powder to the depth of an inch is then sifted over this layer; a new series of bars is next made to fit into the interstices between the first, care being taken that no two bars are in contact, and in this way the troughs are filled to within 6 inches of the top. The filling is then continued with old cement powder, and this is lastly covered with refractory damp sand or fire-tiles, for the purpose of excluding the air, which, if admitted, would greatly injure or altogether stop the process of cementation. The entrances to the furnace being carefully closed, the fire is lighted below the troughs and carefully urged for two, three, or four days, until the proper cementing heat is attained; this heat is maintained during several days more until the Iron has absorbed the quantity of carbon requisite to form the kind of Steel required by the manufacturer.
From six to eight days are sufficient for the production of moderately hard Steel — such, for example, as that known by the name of Shear Steel; softer Steel, for saws and springs, requires a shorter time; harder Steel, for making the chisels used in cutting Iron, takes a longer period; and for some purposes bars are exposed to two or three successive processes of cementation, and are hence said to be twice or thrice converted, In the centre of the end stones of the cementing troughs are small holes, called tasting holes, corresponding with small iron doors in the outer brick work; by these holes the workmen can occasionally draw out a bar to see bow the transmutation is going on. This is judged of by the blisters which appear on the surface of the bars, which give the well-known name of Blistered Steel to this article. When by this process of tasting the change is judged to be complete, the fire is extinguished and the furnace left to cool for about a week, when the process for making blistered Steel is finished. This Steel is very different from the bar Iron from which it was produced. Its surface is covered with blisters, and on breaking a bar across, its texture is seen to be no longer fibrous, but granular or crystalline; the colour is white, like frosted silver, and the crystals are larger in proportion to the amount of the carbon absorbed.
Tilting.
The bar of blistered Steel contains numerous fissures and cavities, which render it unfit for forging, except into a few rough articles. To prepare it for forging into edge-tools and cutting instruments, it requires to be condensed and rendered uniform, which is the object of the next process, called shearing, from being found, soon after its introduction, suitable for making shears ; the process is also called tilting, from the circumstance of a tilt hammer being employed. In some respects the operation of tilting resembles that of shingling in the process of the manufacture of Iron, In the construction of the tilt hammer, the frame-work is strongly secured to the masonry and timber of the foundations, so as to form a firm bed for the block. The shaft of the hammer is made of timber secured by wrought iron rings and fitted into a cast iron socket with trunnions or axles cast upon it, which turn in brasses in a block. The wheel by which the hammer is elevated is furnished with ears or tappits, which, during the revolution of the wheel, engage the end of the shaft and continue to depress it until disengaged, when the hammer head falls with considerable force on the anvil, producing in this way from 150 to 360 strokes per minute. The blistered Steel is prepared for tilting by breaking the bars into lengths of about 18 inches, and binding four or
Please Note: These web pages retain the original pagination from the publication