|
Bentonite This name is given to certain fine-grained clays which are plastic and usually swell enormously when wetted (although some swell only a little more than ordinary clays). A high grade Bentonite, however, will absorb five times its weight of water and will swell to as much as fifteen times its dry bulk. They are employed in moulding sands, oil-well drilling muds, and for various uses in industry. Treatment usually consists of low temperature drying (400 to 500 deg. F.) as the gel-forming properties are injured by temperatures above 750 deg., then crushing in specially designed rolls and finally grinding in ball mills, rod mills or roller mills. Clay Clays are largely composed of silicates of aluminium with impurities of Quartz, Micas and minor quantities of Tourmaline and iron oxides. Roughly, there are two types, the detrital clays, mostly waterborne, although some are of glacial origin, and those of pneumatolytic origin. In both types the chief mineral is Kaolinite, Al2O3 2Si02 2H2O. The China Clays of Cornwall are of the second type, both "potting" and "bleaching" clays being supplied, whilst the ball clays, such as those of Bovey Basin, are of detrital origin and are used for making sanitary ware, as they are less porous when fired. These ball clays are highly plastic, very strong, and are used to impart plasticity to china clays. Fire clays are another variety which are somewhat siliceous and very refractory. Ball clays, filler clays, etc., do not usually receive any treatment, other than drying with disintegration of the dried lumps, in conjunction with screening and air classification for the removal of organic and sandy material. In some cases, the clay is blunged with water, screened at about 200 mesh to remove grit, possibly bleached chemically, thickened, filtered and finally dried to about 3 per cent. moisture. China clays are likewise simply treated, being disintegrated and the fine sand, mica, etc., separated by sedimentation, followed by thickening, filtering and drying. In Cornwall, dispersion is largely obtained by hydraulicing in the pits, but dispersants are sometimes added during treatment for certain classes of clays. Stony material and coarse sand is removed in long settling troughs situated in the pits themselves, but fine sand and mica is settled out in a series of long troughs or "Mica drags" in which the velocity of the stream is caused to decrease whereby different grades of "Mica-clay" are produced. The refined clay leaving the drags is thickened in large conical thickeners and is pumped to filter presses where the moisture is reduced to about 25-30 per cent. From the filter press the cake is conveyed to driers, where the moisture is reduced to under 10 per cent. for most clays, and much less for high-grade products, which are finally disintegrated and packed in paper bags. In the more modern plants the cakes from the filters are conveyed by a creeping conveyor to a knife mill, which shreds the clay on its way to RugglesColes driers, but in the older plants the cakes are trammed by hand to flat hearths, where the clay is dried by long flues beneath them, and finally removed by shovelling. At the time of writing, the older plants are being modernised as quickly as possible, and in a few years it is probable that all the settling pits and mica drags will have given way to rake classifiers and hydro-separators, thickeners and the like. A number of deposits are also worked in North Carolina, but here the clay appears to require more disintegration, and various forms of "Blungers" are used. At the Harris Clay Company's plant at Spruce Pine, the crude clay carries up to 20 per cent. of Kaolin, although averages are only some 12½ per cent. In the Sparks plant the clay is mined by shovels and transported in trucks to a bin, where the crude clay is sluiced to an elevator which delivers it to a blunger consisting of an enclosed trough having a revolving shaft set with teeth 2 ft. long by 1¼ in. sq., and running at 450 r.p.m. From here it is screened, classified and the clay separated as in flowsheet No. 5. Mica is also recovered by flotation of a table product as well as the plus 100-mesh material. The plus 100-mesh passes to four M.S. units, and the concentrate is cleaned in a three-cell Denver unit, whilst the table mica is simply floated in a single Denver cell, both products being dried for use in the roofing-felt industry. At the Lunday plant of the Harris Clay Co., the raw clay is blunged in a Hardinge mill, after which it is classified and dealt with in a very similar manner to the treatment in the Sparks plant. At the Avery-Kaolin plant, on the other hand, roll disintegrators are used, discharging into blungers, from which the coarse fraction is tabled for Mica recovery, whilst the overflow is screened on 50-mesh to remove further Mica which passes to the Mica recovery flotation units, and the undersize from these screens is passed to sand reels and troughs for final sand removal, the final clay being settled and filter pressed. Sand from the reels and troughs are each treated by flotation for Mica recovery, as well as the micaceous fraction from the tables, the concentrate being dewatered in a Fletcher batch centrifuge, and finally dried in a rotary drier at 260 deg. F., yielding a product carrying about one per cent. moisture. This is screened to suit market requirements and sacked. The flowsheet is given in Fig. 6. At the Carolina Clay Co., Fig. 7, separation of the clay is done in sand-wheels, classifiers and settling boxes, after blunging, whilst the Mica is recovered from the sands by jigging after the coarser material has been crushed. Similarly at the Kaolin Incorporated plant, situated at Spruce Pine, North Carolina, the crude clay is first disintegrated in rolls, then treated in a special blunger in which logs, knives and a trommel operate. Gravel is rejected, coarse sand tabled for Mica recovery and the fine sand settled out in reels (comprising a spiral and three sand wheels, in a 5 ft. x 25 ft. trough) and settling troughs. Final clay is screened at 200-mesh, settled, filtered in presses and dried in a tunnel drier. Mica is recovered from the sand residues by flotation, amines, Du Pont 243, a soap, pine oil, sodium silicate and soda ash being reported as reagents used. Corundum Corundum, Al2O3, sp. gr. 4.1 to 3.9 and hardness of 9 (Mohs scale), is an important abrasive material, whilst crystal clear varieties occur in various colours, and are valuable gems such as Ruby, Sapphire, Emerald and Oriental Topaz. Emery, on the other hand, is a mixture of granular Corundum and Magnetite with some Haematite. The treatment has usually consisted of screening and possibly jigging, whilst the Canadian mills used to employ jigs and tables yielding a 55 per cent. concentrate which was dried, treated by magnetic separation and then reconcentrated on tables or pneumatic tables and jigs, and finally reseparated, bringing the ultimate concentrate to 90 to 95 per cent Al2O3. A deposit was worked at Craigmont, Ontario, from 1900 to 1913, where the Corundum occurs in a felspathic syenite associated with Biotite, Muscovite, Magnetite, Hornblende, Garnets, Sodalite, etc., and the tailing stock-piled. This is now being reworked, using a gravity flowsheet, the details of which are given in Fig. 8. Close classification is used before table treatment, and a crown-type pooling riffle is used which is said to result in increased capacity, and to prevent dryness due to crowding on the deck of the tables. These riffles are tapered from 9/16 in. to zero in 3 ft. towards the concentrate end, whilst at the other end the taper is from 9/16 in. to ¼ in, over the remaining length of the riffle. The crude table concentrate is pumped to a Crockett type magnetic separator, where strongly magnetic minerals are removed prior to drying and grading. Diamonds Diamonds are of three different types, the Gem variety, which are transparent, with a high refractive index and dispersion or "fire," dark coloured or poorly crystalline specimens, known as Bortz or Bort, and Carbons or Carbonados, the opaque, dull, imperfectly crystalline variety which possesses a lower specific gravity (3.15 to 3.29, compared with 3.50 to 3.52 for Gem Stones), but are tougher than the more crystalline stones. Treatment consists of crushing, washing, concentration in diamond pans and jigs so that only some one-tenth of one per cent, of the original ore or alluvial is collected in the jigs concentrate. This product is usually rejigged and treated on grease tables. After the grease has been removed, magnetic material is eliminated in a separator before the Diamonds are finally hand picked. A typical flowsheet is that of De Beers Consolidated Mines Ltd., at Kimberley, South Africa, which is shown in Fig. 9. Formerly, the diamondiferous blue ground was subjected to atmospheric weathering for from 4 to 18 months before washing and jigging, when the rock crumbles sufficiently to release the Diamonds. This method, however, is more expensive than conventional crushing, and it has been discontinued, as very few stones are found to be destroyed in the crushers. Felspar
Although Felspar occurs more abundantly than any other mineral, there are rather limited commercial sources, being chiefly granitic pegmatites. Commercial spars may be Orthoclase, K2O Al2O3 6SiO2 Microdine, Albite, Na2O Al2O3 6SiO2, Anorthite, CaO Al2O3 6SiO2 whilst China Stone, known in the States as "Cornwall Stone," is a natural mixture of Felspar, Quartz, some Fluorspar and possibly a little Mica and Kaolinite. This rock is peculiar to parts of the St. Austell district of Cornwall, and is classified into three grades, hard purple, mild purple, white and buff. It is simply crushed and wet-ground in silica-lined ball mills, or in a form of arrastra lined with blocks of china stone. Nepheline, K2O 3Na2O 4Al2O3 9SiO2, is a felspathoid occurring in syenites, and is also sometimes worked for a similar purpose as Felspar. As most Felspar is used for glass, pottery and enamels, it is important that little or no iron is present ; 0.08 per cent. Fe2O3 should not be exceeded. For glass making, granular spar, free from dust, is preferred, and either soda or potash types are used. For pottery the K2O/Na2O ratio is important, too high a soda content is undesirable, particularly for electrical insulators and floor tiles ; but for glazes a high soda spar may be employed. As it is used in a ground state, it is frequently wet ground in this country, although in the United States it is more usually ground dry. and high intensity separators are used for removing abraded iron, Biotite, Garnets, Tourmaline and even some types of Muscovite. Crude spar is frequently hand sorted, crushed in stages, removing Mica as oversize, and finally iron bearing minerals separated in a magnetic separator. Due to the gradual depletion of high grade reserves, combined with more rigid marketing specifications, flotation is being employed commercially to remove impurities and to separate the felspar from quartz. The usual impurities are Mica, Quartz, sulphide minerals, iron oxides, and, to a limited extent, Garnets. Mica may be floated using an amine reagent in a strongly acid circuit, together with aluminium sulphate as a depressor for the fluorspar, whilst the separation of felspar from quartz is effected by depressing the quartz with hydrofluoric acid and floating the felspar with a long chain amine, and an alcohol frother. Unfortunately, this reagent combination leaves much to be desired in so far as cost is concerned, and has not been used extensively. On the other hand, the iron bearing minerals, such as Garnets, as well as iron oxides, may be readily floated from the felspar, using reagents 801 and 825, fuel-oil in a circuit brought to a pH value of about 3.5 with sulphuric acid. Magnetic separation may be employed as an alternative to flotation for the removal of iron bearing minerals, and may be more economic on coarser disseminations. Felspar ores are usually quite abrasive and, as a rule, should be concentrated at a coarse size to meet market requirements. which often demand all minus 20 mesh, with less than 10 or 15 per cent, minus 200 mesh. In consequence, heavy wear may be expected in flotation cells, which is aggravated by the use of hydrofluoric acid at a pH value as low as 2.5, rendering the pulp most corrosive, so that specially moulded rubber wearing parts must be used. For this reason, combined with the usual difficulty in treating coarse material, table agglomeration has been suggested, and excellent separation of felspar from quartz can be made by "Table Flotation" at 12 to 40 mesh. This procedure has the advantage of conditioning in very thick pulps with the possibility of recovering some of the acid before tabling, and in handling coarse material. Flotation is now in commercial operation in California, Tennessee, and North Carolina, and there seems to be no reason why it should not be employed on felspar-rich rocks in this country. The majority of the plants operating, however, simply employ hand picking with magnetic separation. At the Minpro unit of the United Felspar and Mineral Corp. at Spruce Pine, North Carolina, the ore is loaded with forks from the stock bin, so that the fines are separated and stocked for further treatment, whilst the oversize is picked, crushed and dried before stage crushing to 20 mesh in rolls, being finally passed through a magnetic separator. In the fine grinding plant, the various grades of Felspar are blended and ground to the desired fineness, using Hardinge and Tube mills operating in closed circuit with air separators or screens. SELECTED REFERENCES:
Drawings and Photographs accompanying the article
Article reproduced from a copy of the magazine held at National Mining Museum Scotland, Newtongrange, Midlothian.
|
![]() |
||||||||
|
Mail: Webmaster |
Back |
Home |
Copyright © 1999-2024 by The Durham Mining Museum and its contributors Registered Charity No: 1110608 Page last updated: 17 Jan 2023
|
Search |
|
|||